Advanced Composites Handout(Ⅸ):Repair Of Composite Panels

Feb 11, 2025

Leave a message

1,Bonding repair patch

       The fuselage and wing structures of new generation aircraft are made of solid laminates, externally reinforced with co-cured or co-bonded longitudinal beams. These solid laminates have more layers than panels of honeycomb sandwich structures. Stamped repair techniques for solid laminate structures are similar to those for glass fibre, Para-aramid® and carbon fibre, but with minor differences.

      Stamped repairs can be made with a step repair or, more commonly, with a notch repair (tapered repair). The angle of the circumferential cut is usually small to ease the load into the joint and prevent adhesive escape. This translates into a thickness to length ratio of 1:10 to 1:70. Because inspection of bonded repairs is difficult, bonded repairs require a higher commitment to quality control, better trained personnel and cleanliness than bolted repairs.

      From a load transfer standpoint, the embedded joint is more effective because it reduces load eccentricity by closely aligning the female shaft with the neutral shaft of the patch. However, this configuration has a number of disadvantages when performing restorations.

      First, a large amount of acoustic-sensitive material must be removed to maintain a small taper angle.

      Second, the replacement layer must be very accurately laid out and placed in the repair seam.

      Third, the curing of the replacement layer can result in a significant reduction in strength if not cured in an autoclave.

       Fourthly, the adhesive will stick to the bottom of the joint, creating an uneven bond line. This can be mitigated by a series of small steps to approximate the circumferential angle.

       For these reasons, unless the part is lightly loaded, this type of repair is usually performed in a repair facility where the part can be inserted into an autoclave, which can make the part as strong as the original part.

       There are several different repair methods for solid laminates. The patch can be pre-cured and then secondary bonded to the parent material. This method is closest to a bolt-on repair. As shown in Figure 64, a prepreg can be made into a patch and then co-cured at the same time as the adhesive. Patches can also be repaired using a wet lay-up layer. The curing cycle can also vary in length of time, curing temperature and curing pressure, increasing the number of possible repair combinations.

news-266-128

Figure 64: Pre-cured patches can be secondarily bonded to the primary substrate

2,Repair of composite bevelled panel

     Step 1: Damage inspection and survey

     The size and depth of the damage to be repaired must be accurately measured using appropriate non-destructive evaluation (NDE) techniques. A variety of NDE techniques can be used for damage inspection of composite structures. The simplest technique is visual inspection, where whitening due to delamination or resin cracking in translucent composites such as glass-polyester and glass-vinyl ester laminates can be used to indicate areas of damage.

     Visual inspection is not an accurate technique as not all damage can be detected by the eye, particularly damage hidden by paint, damage located deep below the surface, and damage in non-transparent composites such as carbon fibre and aramid laminates. A popular technique is the tap test, where a lightweight object, such as a coin or hammer, is used to locate damage. The main benefit of the tap test is that it is simple and can be used to quickly inspect large areas. Tap testing is typically used to detect delamination damage close to the surface, but it becomes less reliable as the delamination is located at depths below the surface. The cone tap test is not useful for detecting other types of damage, such as resin cracks and broken fibres.

      More advanced NDE techniques for detecting composites are impedance testing, x-ray radiography, thermography, and ultrasound. Of these techniques, ultrasound is arguably the most accurate and practical and is often used to measure damage. Ultrasound can be used to detect small layers located below the surface, unlike visual inspection and percussion testing.

     Step 2: Remove Damaged Material

     Once the extent of the damaged area to be repaired has been determined, the damaged laminate must be removed. The edge of the sound source laminate is then tapered to a shallow angle. The taper slope ratio, also known as the circumferential angle, should be less than 12:1 (<5°) to minimise shear strain along the bondline after repairing the patch. The shallow angle also compensates for some errors in process and other operational variables that may reduce patch adhesion. As shown in Figure 65.

news-266-280

Figure 65: Embedded patch solid laminated board

      Step 3: Surface Preparation

      The laminate near the embedding area should be lightly sanded with sandpaper and then dust and contaminants should be removed. It is recommended that if the embedding area has been exposed to the environment for a considerable period of time, it should be cleaned with a solvent to remove contamination.

     Step 4: Forming/Film Tooling

     A rigid support plate with the original contours of the composite structure is required to ensure that the repair has the same geometry as the surrounding structure.

     Step 5: Lamination

      Laminated repairs are typically made using a minimal sequence of ply-preferred tapers. While this repair is acceptable, it produces relatively weak resin-rich areas at the edges of each layer at the repair interface. The maximum thickness first ply lamination sequence, where the first layer of reinforcing fabric completely covers the working area, produces a stronger interfacial connection. It follows the manufacturer's SRM instructions.

     The choice of reinforcement material is critical to ensure that the repair has acceptable mechanical properties. The reinforcing fabric or tape should be the same as the reinforcing material used in the original composite.

     The fibre orientation of the reinforcement layer within the repair plywood should match that of the original part plywood so that the mechanical properties of the repair are as close as possible to those of the original material.

3,Repair of wing trailing edges and transition areas

      The trailing edge of the wing of the control panel is very susceptible to damage. The trailing 4 inches are particularly vulnerable to ground impact and handling, as well as lightning strikes. Repairs can be difficult in this area because skinning and trailing edge reinforcement may be involved. Repairs to honeycomb cores on damaged edges or panels are similar to repairs requiring core replacement and damaged sandwich honeycomb structures discussed in one or both panel repair sections. The damage is investigated, damaged layers and cores are removed, the part is dried, a new core is installed, a repair layer is applied, cured and inspected after repair. A typical wing trace edge repair is shown in Figure 66.

news-266-324

Figure 66: Repair of wing trailing edge

4,Repair by resin injection

      Resin injection repair is used for solid laminates of light duty construction with small damage due to delamination. Two holes are drilled on the outside of the delamination area and low viscosity resin is injected into one of the holes until the resin flows out of the other hole. Resin injection repair is sometimes used in sandwich honeycomb structures to repair panel detachment. The disadvantage of the resin injection method is that it is difficult to remove moisture from the damaged area due to the fibres being cut off as a result of the drilling, making it difficult to achieve complete resin injection, as shown in Figure 67.

news-266-170

Figure 67: Repair by resin injection

To be continued